Preventing Crazing & Cloudiness During CNC Polycarbonate Machining
A common mistake in polycarbonate machining is spraying petroleum- or ester-based cutting oils, which trigger micro-crazing inside the polymer chains within hours. Jeton strictly machines clear PC dry with chilled clean air or water-soluble inert mist, uses polished diamond-like carbide cutters to leave translucent toolpaths ready for multi-stage wet polishing or vapor smoothing, and runs a controlled 115°C annealing bake on threaded bosses.
Engineering Specs & Design Rules for Machined PC Parts
- Optical Finishing Options: Translucent frost (bead blast), satin semi-clear, manual multi-grit optical polish, or vapor polishing up to 89% clarity.
- Chemical Resistance Caution: PC resists dilute acids and alcohols briefly but cracks under ketones, acetone, and strong alkaline cleaners—consider PSU/PPSU or Tritan/PCTG if repeatedly autoclaved.
- Thread & Fastener Guidance: Avoid coarse self-tapping screws in tight PC bosses without stress-relief annealing; specify M2–M4 brass inserts or cut fine machine threads.
- Injection Molding Scale-Up: Translates directly into NAK80 SPI A1/A2 mirror steel molds (0.5%–0.7% shrinkage) for clear light diffusers.
PC vs. PMMA Acrylic vs. PC/ABS: Quick Engineer Decision Rule
Choose PC when drop-test toughness and 120°C heat deflection outrank scratch hardness; pick PMMA acrylic when crystal-clear 92% optics and UV weatherability come first; select opaque PC/ABS when UL94 V-0 flammability plus easy chemical resistance in chargers or auto interiors is required.